Blue enamel on glass: an investigation into microfracturing and material loss of 17th century copper and cobalt blue enamel
TitelBlue enamel on glass: an investigation into microfracturing and material loss of 17th century copper and cobalt blue enamel
Verantwoordelijkheids-vermeldingRoy van der Wielen
Verantwoordelijke(n)
Plaats van uitgave[S.I
Uitgevers.n.]
Jaar van uitgaveJune 2017
Pagina's1 online resource (PDF, 81 pagina's)
Illustratiesillustraties
MateriaalDigitale publicatie ; Scripties
SamenvattingThe Rijksmuseum Amsterdam owns a collection of fractured 17th century enamelled glass panels that have been mended with clear tape consisting of a cellophane carrier and rubber adhesive. In many cases, this tape has been applied over the decorated side and has yellowed and shrunk. Future removal of this tape instigated the investigation of the condition of these objects.
In this thesis, the focus was laid on microfractures and the subsequent loss of blue enamel on three panels: BK. LXXX II d., BK. LXX b. and BK. LXXXI i.
XRF-analyses identified copper based and cobalt based enamel with a similar lead and potassium flux. The used carrier glass was High Lime Low Alkali (HLLA) glass.
The identified degradation phenomenon was a network of vertical surface microfractures crossing both the enamel as well as a proportion of the carrier glass. These microfractures are interconnected in the horizontal plane, undermining areas of the glass carrier and blue enamel. In this research, the term ‘cross-phase microfracturing and subsequent flaking’ was used to describe this phenomenon. On the three objects, the condition of cobalt blue enamel seemed significantly better than that of copper blue enamel.
In contemporary conservation literature, cross-phase microfractures and subsequent flaking is believed to be the result of tension, caused by a discrepancy in the thermal expansion coefficients of the enamel glass and the carrier glass . By visually investigating basic fractographic characteristics, this hypothesis was found plausible. However, insufficient explanation for significant difference in condition between copper and cobalt blue enamel on the Macaw panel was offered.
Numerous surface pits and gas inclusions have been found in copper blue enamel layers, that were almost absent in cobalt blue enamel. The presence of these seems to be related to the formation of cross-phase microfractures, although the nature of this relation is unclear. Literature agrees that the presence of gas inclusions implicates that the enamel has not melted properly. The melting point of a glass is determined by added fluxing agents. The flux ratio in both enamel types did not differ in such a way that would result in two different melting points. However, cobalt blue enamel contained arsenic contaminations. Arsenic is claimed to be a powerful flux and has the capacity to remove gas inclusions from a molten glass. It was concluded that influence of arsenic on the durability of blue enamels deserves further investigation.
The identification of thermally induced microfractures is relevant for conservation. When removing tape, care should be taken not to lose material. Another possible scenario would be shrinking cellophane backing tearing off material.
The diagnosed degradation phenomenon will progress unless temperature fluctuations are kept to a minimum.
In this thesis, the focus was laid on microfractures and the subsequent loss of blue enamel on three panels: BK. LXXX II d., BK. LXX b. and BK. LXXXI i.
XRF-analyses identified copper based and cobalt based enamel with a similar lead and potassium flux. The used carrier glass was High Lime Low Alkali (HLLA) glass.
The identified degradation phenomenon was a network of vertical surface microfractures crossing both the enamel as well as a proportion of the carrier glass. These microfractures are interconnected in the horizontal plane, undermining areas of the glass carrier and blue enamel. In this research, the term ‘cross-phase microfracturing and subsequent flaking’ was used to describe this phenomenon. On the three objects, the condition of cobalt blue enamel seemed significantly better than that of copper blue enamel.
In contemporary conservation literature, cross-phase microfractures and subsequent flaking is believed to be the result of tension, caused by a discrepancy in the thermal expansion coefficients of the enamel glass and the carrier glass . By visually investigating basic fractographic characteristics, this hypothesis was found plausible. However, insufficient explanation for significant difference in condition between copper and cobalt blue enamel on the Macaw panel was offered.
Numerous surface pits and gas inclusions have been found in copper blue enamel layers, that were almost absent in cobalt blue enamel. The presence of these seems to be related to the formation of cross-phase microfractures, although the nature of this relation is unclear. Literature agrees that the presence of gas inclusions implicates that the enamel has not melted properly. The melting point of a glass is determined by added fluxing agents. The flux ratio in both enamel types did not differ in such a way that would result in two different melting points. However, cobalt blue enamel contained arsenic contaminations. Arsenic is claimed to be a powerful flux and has the capacity to remove gas inclusions from a molten glass. It was concluded that influence of arsenic on the durability of blue enamels deserves further investigation.
The identification of thermally induced microfractures is relevant for conservation. When removing tape, care should be taken not to lose material. Another possible scenario would be shrinking cellophane backing tearing off material.
The diagnosed degradation phenomenon will progress unless temperature fluctuations are kept to a minimum.
AnnotatieMet samenvatting in het Nederlands ; With summary in English
Met literatuuropgave (pagina's 68-70).- Alleen digitaal beschikbaar
Master thesis Conservation and Restoration of Cultural Heritage, Specialization: Glass, Ceramic and Stone, University of Amsterdam, 2017
Met literatuuropgave (pagina's 68-70).- Alleen digitaal beschikbaar
Master thesis Conservation and Restoration of Cultural Heritage, Specialization: Glass, Ceramic and Stone, University of Amsterdam, 2017
TrefwoordenUvA Scripties, emaille, gebrandschilderd glas, restauratie, conservering